Equipment / Silica sand laboratory assay

Silica sand iron removal: dry, wet and acid washing assay results

This page presents laboratory assay results for a silica sand sample after dry magnetic separation, wet magnetic separation, and wet magnetic separation followed by acid washing.

Wet magnetic separation combined with acid washing upgraded the sample to 99.87% SiO₂ and sharply reduced Al₂O₃ and TiO₂. Fe₂O₃ was reduced from 0.027% (270 ppm) in the raw ore to 0.011% (110 ppm). This is still above a typical low-iron target of 80 ppm. Remaining iron may be locked inside quartz grains or present in an acid-resistant mineral form.

All figures apply strictly to this tested sample and do not serve as a commercial plant guarantee. Final process selection should be confirmed by sample testing.

Key assay results

The summary table below is a laboratory assay of the tested sample. A dash (—) means that item was not reported at that stage. Fe₂O₃ conversion: 0.001% = 10 ppm. A typical low-iron target of Fe₂O₃ ≤ 80 ppm is shown for reference only.

Key assay results for a tested silica sand sample: raw ore, dry magnetic separation, wet magnetic separation, and wet magnetic separation plus acid washing
Key results for this tested sample — dry, wet, and wet magnetic separation followed by acid washing. Figures apply only to this tested sample and are not a commercial plant guarantee.
Stage SiO₂ (%) Fe₂O₃ (%) Fe₂O₃ (ppm) Al₂O₃ (%) TiO₂ (%) LOI / IL (%)
Raw Ore 98.32 0.027 270 0.91 0.12 0.48
Dry Magnetic Separation 98.86 0.019 190 — — —
Wet Magnetic Separation 99.45 0.013 130 — — —
Wet Magnetic Separation + Acid Washing 99.87 0.011 110 0.025 0.0047 0.020

After wet magnetic separation and acid washing, Fe₂O₃ is 0.011% (110 ppm). That is still 30 ppm above a typical low-iron target of 80 ppm. This page does not state that the 80 ppm target was met, and it does not claim that a stronger acid-washing step would necessarily reach 80 ppm.

Route A and Route B

Two routes were recorded on this sample. Acid washing was applied only after wet magnetic separation (Route B). It was not applied after dry magnetic separation, and it was not applied on both routes.

  • Route A: silica raw ore → dry magnetic separation. After dry magnetic separation, SiO₂ was 98.86% and Fe₂O₃ was 0.019% (190 ppm).
  • Route B: silica raw ore → wet magnetic separation → acid washing. After wet magnetic separation, SiO₂ was 99.45% and Fe₂O₃ was 0.013% (130 ppm). After the subsequent acid washing, SiO₂ was 99.87% and Fe₂O₃ was 0.011% (110 ppm).
Laboratory assay comparison for a tested silica sand sample, showing Route A dry magnetic separation and Route B wet magnetic separation followed by acid washing
Full laboratory assay comparison for this tested sample. Route A is dry magnetic separation only. Route B is wet magnetic separation followed by acid washing.

Additional oxides reported on this sample

On the raw ore, the laboratory also reported CaO 0.023%, MgO 0.0059%, K₂O 0.0042% and Na₂O 0.0070%. After wet magnetic separation and acid washing, the same items were CaO 0.0033%, MgO 0.0021%, K₂O 0.0036% and Na₂O 0.0036%. These values were not reported for the dry-magnetic-separation stage or for the wet-magnetic-separation stage alone.

How to read these figures

This is a laboratory assay of the tested sample. The figures are not a plant performance result and do not serve as a commercial plant guarantee. They do not identify a project, a customer or a laboratory, and they are not tied to a report number or a test date on this page.

A typical low-iron target of Fe₂O₃ ≤ 80 ppm is shown only as a reference. On this sample, Fe₂O₃ after wet magnetic separation and acid washing remained at 110 ppm, which is still above that target.

Related process context for silica sand lines is published on the silica sand line page. Configuration for a given ore is confirmed by sample testing. We offer a free 5–10 kg lab test; the report is issued within 5 days of receiving the sample. Price on request.

Frequently asked questions

Was acid washing applied after both dry and wet magnetic separation?

No. On this sample, acid washing was applied only after wet magnetic separation (Route B). Route A is dry magnetic separation only.

Did Fe₂O₃ reach the 80 ppm target?

No. After wet magnetic separation and acid washing, Fe₂O₃ was 0.011% (110 ppm), which is still 30 ppm above a typical low-iron target of 80 ppm. This page does not state that a stronger acid-washing step would necessarily reach 80 ppm. Remaining iron may be locked inside quartz grains or present in an acid-resistant mineral form.

Do these figures apply to a production plant?

No. All figures apply strictly to this tested sample and do not serve as a commercial plant guarantee. Final process selection should be confirmed by sample testing.

How can another silica sand sample be tested?

Send 5–10 kg for a free lab test. We deliver a report within 5 days of receiving the sample. Results apply to the sample received and the recorded conditions. Price on request.

Need a test on your silica sand?

Send a 5–10 kg sample for a free laboratory test. The report is issued within 5 days of receiving the sample. Results apply to the sample received. Price on request.